Chenfan Electric
EN
Send drawing

ARTICLETechnical article

Keeping Mill Welds Out of Finished Core Laminations

  • Chenfan Power

Keep each identified coil weld and its approved surrounding exclusion region outside the finished lamination. Establish the weld reference from the incoming material record and qualified detection, then carry its corrected position through the cutting plan.

Calculation basis. Numerical demonstrations use editorial assumptions unless a value is expressly attributed to a cited supplier, standard or published study. Dimensions describe the stated model geometry; test results introduced with “assume” or “suppose” are hypothetical inputs. Calculated outputs inherit those conditions.

The important decisions are where the weld reference came from, how its position reaches the cutter and what happens when the position or detection status is uncertain. A sensor output and an exclusion interval are separate pieces of evidence.

Establish the origin of the weld reference

Ask what the supplied record actually identifies: a joining weld, a physical marker, an approximate length position or an inspected weld-center coordinate. Retain the parent material identity and coordinate origin. A painted mark is not automatically coincident with the metallurgical weld center, and a supplier’s length record is not automatically registered to the line’s current encoder zero.

Distinguish an incoming mill weld from a splice introduced during subsequent processing. If the route permits joining material, that new feature needs its own identity and position record. Where the purchasing definition requires unwelded supplied material, an unexplained weld is a conformity issue rather than something the cutting algorithm may silently accommodate.

Define the prohibited physical interval from the approved transformer-core material and part requirements. Set the detector threshold for the qualified detection task and keep it separate from metallurgical acceptance.

Qualify detection on representative material

Qualify the detector on representative welded and unwelded material from the intended grade, thickness, coating and line route. Retain the detector configuration, speed range, material spacing and the reference used to establish the weld centre.

Assess seam detectability separately from located-event accuracy. Test missed-event behaviour and output timing; a larger position margin cannot compensate for a seam that generates no event.

Use known representative weld samples and unwelded comparison material to challenge the actual configured system. Include the applicable operating conditions and startup state. A reported detection event should be traceable to the configuration that generated it. Missing a seam and locating a detected seam inaccurately are different failure modes; a position margin addresses only the latter.

Account for the delay between passage and report

Position must refer to the physical feature and its time reference. Characterize the complete detector-to-controller delay and its variation under the intended line conditions, then determine whether the captured coordinate already contains compensation.

Characterize the complete route: sensor response, filtering, output switching, input acquisition, event timestamp and position capture. If position is captured at the report rather than the underlying physical reference, identify the necessary correction and its uncertainty. Do not add a correction twice when the qualified system already provides compensated event coordinates.

For variable speed, distance traveled during a delay is the time integral of actual strip speed over that interval. A fixed time compensation based on one nominal speed can become wrong during acceleration or deceleration. The position reference must also follow the strip; uncharacterized measuring-wheel slip cannot be removed by an exact PLC timestamp.

Hypothetical weld timing calculation and a lamination footprint overlapping a bounded exclusion interval by 10 mm.
Hypothetical constant-speed event timing and a separate one-dimensional exclusion test. Total event delay is assumed to be 80 ms; it is not a cited detector rating. The corrected center has an assumed ±30 mm residual position bound, enlarging an approved ±100 mm physical zone to ±130 mm. A lamination center outside that interval does not prove its full length is clear.

A hypothetical timing and exclusion calculation

Suppose the weld center crosses an upstream sensor at t = 0, the cutter is 2.00 m downstream, speed is a constant 0.50 m/s, and the complete qualified event delay is 0.080 s. These are assumed teaching values and are not specifications of either cited detector.

At the report time, the weld has advanced 0.50 × 0.080 = 0.040 m. Its remaining travel to the cutter is 1.960 m, corresponding to 3.920 s at that speed. Waiting a further 2.00/0.50 = 4.000 s from the delayed report would be 0.080 s late, equivalent to 40 mm of strip travel. This checks the sign of the compensation; it is not a command schedule for an operating cutting line.

Separately suppose the approved physical exclusion half-length is 0.100 m and the qualified bound on residual center-position error after compensation is ±0.030 m. The conservative planning interval is then ±0.130 m about the reported, corrected weld coordinate: total length 0.260 m. This uses a bounded position error, not a standard uncertainty or a statistical confidence interval. The 30 mm allowance is assumed to include the relevant residual tracking errors; adding an already included component again would double-count it.

Compare the whole intended lamination footprint with that interval. In this one-dimensional teaching model, a lamination occupying −0.250 to −0.120 m relative to the corrected center intersects the prohibited interval from −0.130 to −0.120 m. Its center lies outside, but 10 mm of its length remains inside. A center-only check would incorrectly clear it.

Keep uncertainty and scrap disposition visible

An approved control needs more than one successful detection. Retain the coordinate event, compensation definition, exclusion rule and the identities of every affected piece. Resolve what happens during missed-event indications, sensor faults, startup, loss of tracking and material identity changes under the qualified line procedure.

Do not interpret a larger exclusion region as protection against a completely missed weld: without a located event, there is no known interval around which to apply it. Likewise, absence of an alarm is not proof that a coil was unwelded. That conclusion needs the supplier record and the validated detection coverage appropriate to the material route.

Verify containment of the identified weld region and reconcile every affected piece with its physical disposition. Release laminations against the approved material definition using the linked detection event, spatial exclusion record and material identities.

Translate the weld exclusion into rejected steel

Nippon Steel lists 23ZH90 at a nominal steel thickness of 0.23 mm and an assumed density of 7.65 kg/dm³. [1] For an assumed 300 mm strip width and the calculated 260 mm exclusion length, nominal rejected steel mass is 0.300 × 0.260 × 0.00023 × 7,650 = 0.137241 kg. Rejecting only the assumed 200 mm physical weld zone would remove 0.105570 kg and omit the 0.031671 kg represented by the tracking margins. Release the expanded interval in the cut plan, then record the actual affected pieces and their scrap disposition.

Manufacturing controls. Control weld-reference location, detector qualification, strip-speed history, delay correction, measuring-wheel slip and cutting registration. Margin size is a position-control decision; detection coverage needs its own challenge test.

IEC 60404-8-7 covers supplied grain-oriented electrical-steel magnetic and geometric characteristics. Carry the approved supplied grade and dimensional basis into this manufacturing record. [2]

References

[1] Nippon Steel Corporation, Grain-Oriented Electrical Steel Sheets, undated, specification tables and annealing compatibility.

[2] IEC, IEC 60404-8-7:2020, Magnetic materials — Part 8-7: Specifications for individual materials — Cold-rolled grain-oriented electrical steel strip and sheet delivered in the fully-processed state.

Chenfan Electric

Direct coordination

Start a conversation.

A drawing, a material requirement, or a project to discuss.

Send drawing