Qualify interlaminar friction on the actual coating, normal load and intended slip plane. Preserve oil, thermal and handling history in the test, then transfer the result through the assembly’s documented shear path.
Calculation basis. Numerical demonstrations use editorial assumptions unless a value is expressly attributed to a cited supplier, standard or published study. Dimensions describe the stated model geometry; test results introduced with “assume” or “suppose” are hypothetical inputs. Calculated outputs inherit those conditions.
Begin with a load-path drawing. Identify which sheet or packet can move, which interfaces resist that movement and how the normal force reaches each interface. That drawing prevents a common error: multiplying one interface’s resistance by the number of sheets when the shear load passes through interfaces in series.
Preserve the surface state being investigated
Use the actual coating and material orientation, with the relevant thermal and handling history. Record cleaning, oil or other contamination, wear and whether the specimens have already slid. Abraded steel-to-steel contact is a different interface from intact insulation-coated sheets.
Define normal pressure, contact footprint and their uniformity. A nominal applied force divided by the drawing area is only an average; tilt, waviness or local seating can change contact. Retain temperature, dwell, sliding direction and speed. Keep those conditions with the identified contact law.
Pirnat, Čepon and Boltežar’s original laminated-structure study varied electrical-steel stacks, treatments and clamping states while identifying dynamic contact parameters. It establishes that surface and assembly choices matter. Its tangential stiffness and damping parameters are not static or kinetic Coulomb coefficients, and should not be entered into a slip calculation as though they were. [2]
Measure initiation and continued movement separately
In a defined pull-out or direct-shear test, retain force and relative displacement between the contacting pieces. Crosshead movement also includes fixture deformation and grip motion. Check the normal-force record throughout the pull rather than assuming it remains at its initial setting.
Identify a reproducible movement criterion for initiation. A force peak may include fixture drag, edge interference, coating adhesion or a geometric snag. It is not automatically a pure friction peak. After movement begins, retain resistance as a function of displacement and speed rather than selecting one convenient low point.
Static friction can supply the required interface force up to its limiting capacity, while the simplified sliding law opposes actual relative motion. This distinction matters in an assembly model. Before slip, the friction force is not always equal to mu_s N; that is a bound, not an imposed load.
A constant kinetic coefficient is also an approximation. If resistance changes with sliding distance or repeated cycles, preserve that evidence and select a model able to represent the relevant behavior.
Count the coupon’s contact faces correctly
For a middle sheet pulled between two fixed sheets, both faces can resist movement. After correcting identified fixture contributions, the simple model is F_resistance = mu_top N_top + mu_bottom N_bottom. It assumes Coulomb-like contact, known normal forces and no extra edge or bond resistance.
For an illustrative symmetric test, let each face carry N = 500 N. Assume an initiation resistance of 300 N and a subsequent sliding resistance of 200 N. With two equivalent faces, mu_s = 300/(2 × 500) = 0.30 and mu_k = 200/(2 × 500) = 0.20. These are assumed observations used for arithmetic, not measurements of a coating or expected CRGO coefficients.
Treating the 300 N pull as a single-face resistance would give 0.60 and double the inferred coefficient. Conversely, dividing a genuinely single-interface shear test by two would understate it. Record the fixture’s actual contact topology beside the reported result.

Translate the result through the packet’s shear path
For one potential sliding interface, a simplified static bound is R = ∫mu_s(x) p(x) dA over its actual contact area. If a constant coefficient represents that entire contact, the bound reduces to mu_s N. Local separation and mixed surface states can invalidate that simplification.
Consider an assumed shear load Q = 250 N transmitted successively through two packet interfaces. Each has a normal force of 1200 N. If their static coefficients are 0.30 and 0.18, their simple capacities are 360 N and 216 N. The second interface fails the assumed no-slip bound even though the first passes it. Adding the capacities to obtain 576 N would be wrong for this serial load path.
Separate interfaces can add resistance when they act in parallel against the same moving body, as in the two-face coupon. Their load sharing must still be justified. The assembly’s restraint and applied shear location determine whether the interfaces are serial, parallel or a more complicated network.
The arithmetic supplies neither a safety factor nor a release criterion. Those require actual test variability, service loads, maintained normal force and design-specific evidence.
Validate the extrapolation to the assembled packet
A small coupon may remove sheet waviness, packet edges, restraints or joining features present in the real assembly. A bonded packet can transmit shear through adhesion as well as friction. Do not hide those mechanisms inside a coefficient labeled as a material constant.
Szabó and colleagues report shear response changing with normal preload in a complete motor rotor stack. Use a representative transformer-core packet to qualify any coupon-to-assembly extrapolation. [3]
The author-proposed handover joins surface history, contact topology, normal-load observations, initiation and sliding records, repeat variability and the intended assembly slip plane. Keep a dynamic vibration fit separate from a large-slip qualification.
Identify the potential slip interface, its maintained normal force and the observation supporting its resistance. Check that interface against the transmitted shear load, with assembly variability and the required design margin included in the qualification.
Recheck the no-slip screen with the actual lower packet
Nippon Steel lists 23ZH90 at a nominal steel thickness of 0.23 mm and an assumed density of 7.65 kg/dm³. [1] Assume 100 sheets of 300 × 500 mm form the lower subpacket. Nominal steel mass is 26.3925 kg. At an assumed in-plane acceleration of 4 m/s², the shear demand is 105.57 N. With an assumed static coefficient 0.18 and normal force 500 N, capacity is 90.00 N, a 15.57 N deficit. A design review must change the verified load path or its controlled inputs before that acceleration case is accepted.
Manufacturing controls. Control the coating state, contact topology, normal-force distribution, lower moving mass and acceleration. Identify static initiation and post-slip response separately; fitted dynamic-contact parameters are not Coulomb coefficients. [2]
References
[1] Nippon Steel Corporation, Grain-Oriented Electrical Steel Sheets, undated, specification tables and annealing compatibility.
[2] M. Pirnat, G. Čepon and M. Boltežar, Introduction of the linear contact model in the dynamic model of laminated structure dynamics: an experimental and numerical identification, 2013, DOI 10.1016/j.mechmachtheory.2013.02.003.
[3] V. Szabó, D. Harrach, D. Feszty and B. Pere, A Method for Measuring Normal and Shear Stiffness of Laminate Stacks of Electric Motors, 2023, DOI 10.3311/PPme.20505.