Set wound-core bend radius through three checks: local lamination strain, the material yield screen and controlled magnetic tests after the qualified manufacturing route. That connects a measurable forming geometry to the core performance the buyer needs.
The decision is whether a proposed radius produces a repeatable magnetic result after the approved manufacturing route. A radius selected only because the strip can be formed without breaking has not answered that question.
Use the radius of one lamination
For an initially flat strip in approximately pure bending, let t be steel thickness, rᵢ the inside surface radius and Rₙ the neutral-layer radius. With a symmetric section and negligible membrane tension:
Rₙ ≈ rᵢ + t/2
ε(y) ≈ y/Rₙ; |εₛ| ≈ t/(2Rₙ) = t/(2rᵢ + t)
Here y is the distance from the neutral layer, positive toward the convex face; strain ε is dimensionless. Compare each surface arc length with the neutral-layer arc length to obtain the expression. The convex face is in tension and the concave face in compression.
Two distinctions matter. First, the inner and outer faces of one sheet have opposite strain signs. Second, sheets nearer the inside of the wound packet generally have smaller local radii and greater strain magnitudes. These are different comparisons. Use each lamination’s curvature; substituting the whole packet thickness assumes a bonded composite section that a sliding lamination stack has not established.
The formula assumes an initially flat, stress-free reference. If the strip already has curvature, use the curvature change: ε(y) ≈ y(κfinal − κinitial), with κ = 1/R. Applied strip tension adds a membrane-strain contribution. Springback, asymmetric coatings and plastic deformation can also change the neutral-layer position. The simple formula therefore screens a geometry; it does not reconstruct an unknown forming history.
Separate first yield from a magnetic acceptance limit
Within a linear elastic model, σ(y) = Eε(y), where E is the modulus in the direction being bent. Grain-oriented steel is mechanically anisotropic: an arbitrary generic steel modulus is a poor substitute for material-specific data.
An initial yield screen is:
εᵧ = σᵧ/E; Rₙ,first yield ≈ Et/(2σᵧ)
Here σᵧ is the relevant yield strength. In ideal symmetric elastic–plastic bending, the central zone remains elastic while outer zones yield; its half-thickness is approximately yᵧ = σᵧRₙ/E, capped at t/2. This describes a model during loading, not the residual stress profile after unloading. Actual hardening and tension–compression differences require a suitable constitutive model.
Above yield, continuing to multiply strain by E gives an elastic trial stress, not a credible actual stress or residual stress. Equally, a radius that passes the yield screen is not automatically magnetically acceptable: maintained elastic restraint can still change the magnetic response.
An independently reproducible radius screen
Assumptions: an initially flat 0.23 mm strip, no membrane tension and symmetric tension/compression yield behaviour. Use representative rolling-direction E = 122,000 MPa and yield strength σᵧ = 331 MPa from Cleveland-Cliffs Table 3; the catalogue describes these as representative, rather than guaranteed grade properties. [1]
| Inside radius rᵢ | Neutral radius Rₙ | Surface strain magnitude | Elastic trial stress Eεₛ | First-yield screen |
|---|---|---|---|---|
| 20 mm | 20.115 mm | 0.572% | 697 MPa | Exceeds assumed yield |
| 40 mm | 40.115 mm | 0.287% | 350 MPa | Slightly exceeds assumed yield |
| 80 mm | 80.115 mm | 0.144% | 175 MPa | Below assumed yield |
For the 20 mm case, εₛ = 0.23/(2 × 20 + 0.23) = 0.005717, or 0.572%. The first-yield strain is 331/122,000 = 0.002713, or 0.271%. The corresponding inside-radius screen is 122,000 × 0.23/(2 × 331) − 0.23/2 = 42.27 mm.
That last number is a result of these assumptions, not a recommended minimum bend radius. The 40 mm case sits close enough to the assumed boundary that actual material properties and tension could change the classification. None of the three rows predicts watts per kilogram or an annealing recovery percentage.

Pair magnetic measurements around the thermal step
Use material from the same coil region and preserve specimen identity. A practical trial has formed specimens at the candidate radius, tested before and after an approved stress-relief treatment, plus matched reference specimens receiving the same thermal treatment. A large-radius reference can reduce bending severity, but remains a geometric reference rather than perfectly unstressed steel. Retain unheated references to detect measurement drift.
At a selected operating peak induction and 50 or 60 Hz, record specific loss, the corresponding excitation response and the actual induction waveform. Keep the winding arrangement, magnetic-path convention, steel cross-section, mass normalization, temperature, joint state and mechanical restraint reproducible. Repeat mounting sufficiently to estimate setup variation; repeated readings on one core do not become independent cores.
For specimen i, report the paired change Δpᵢ = pafter,i − pbefore,i, in W/kg. A negative value indicates lower measured loss under the matched conditions. Compare it with the reference change and with measurement uncertainty. If the reference also improves substantially, thermal treatment has affected the reference state; assigning all improvement in the tight-radius specimen to bending-stress relief would overstate the evidence.
A treatment can also alter restraint, geometry or insulation condition. Record those changes alongside the magnetic data. Do not flatten an annealed curved specimen merely to fit a conventional material fixture and assume its bending history is preserved: that operation introduces another deformation history.
Separate forming-related recovery from the common thermal change
Assume matched tests at 1.7 T, 50 Hz and 20 °C: a formed specimen changes from 1.20 to 1.02 W/kg, while its matched large-radius reference changes from 1.00 to 0.96 W/kg. The changes are −0.18 and −0.04 W/kg, so the difference in changes is −0.14 W/kg. Assume four independent standard uncertainties of 0.01 W/kg; their combined value is 0.02 W/kg, or 0.04 W/kg expanded with an assumed k = 2 [2]. The resulting −0.18 to −0.10 W/kg interval resolves an additional reduction in the formed specimen. Correlated errors require covariance. This comparison supports the stated paired trial, rather than a universal recovery percentage or a minimum production radius.
Release the radius together with the process state
Stress-relief annealing is a material- and coating-specific process. The Cleveland-Cliffs brochure explicitly distinguishes its GO products’ treatment from procedures for other electrical steels and warns that thermal gradients can reintroduce stress. Follow the steel producer’s approved route; this article does not prescribe a furnace cycle. [1]
Release documentation should identify the grade and thickness, radius definition and measured range, forming history, approved thermal route, final restraint state and magnetic acceptance conditions. A material test characterizes its specimen; a finished-core test additionally includes joints and assembly geometry. Keep those acceptance levels separate.
Release the radius against the measured magnetic result for the stated material, forming route and thermal process. Use strain screening to select the trial geometry and paired tests to quantify magnetic recovery.
Control forming and heat treatment together
Inside radius, strip tension, sheet gauge, mandrel alignment and final restraint control the strain history. Nippon Steel also identifies cutting, punching and bending stresses as causes of magnetic deterioration, and requires the annealing route to match the processing and core specification. [3] Preserve coating identity and the actual furnace record with the final-state core test.
References
- Cleveland-Cliffs, LITE CARLITE and Mill-Anneal Grain-Oriented Electrical Steels, October 2023, Table 3 and Stress-Relief Annealing.
- B. N. Taylor and C. E. Kuyatt, NIST Technical Note 1297, Guidelines for Evaluating and Expressing the Uncertainty of NIST Measurement Results, 1994, sections 5 and 6.
- Nippon Steel Corporation, Grain-Oriented Electrical Steel Sheets, catalogue D004je, April 2020, specification tables, size tolerances and Annealing by Customers.